服務(wù)熱線電話
400-6188-756
高壓水沖完毛刺,零件為什么反而生銹了
來源:http://m.sflrw.com/ 時(shí)間: 2026-10-12 瀏覽次數(shù): 0
CNC加工件用高壓水射流去完毛刺,表面看著光潔干凈,放了一兩天,邊角和孔口出現(xiàn)銹點(diǎn)。有的零件甚至當(dāng)天就泛黃。車間以為是水質(zhì)問題,換了純水還是銹。排查下來,問題出在高壓水沖擊之后的表面狀態(tài)。
CNC machined parts are deburred with high-pressure water jet, and the surface looks smooth and clean. After one or two days, rust spots appear on the corners and holes. Some parts even turn yellow on the same day. The workshop thought it was a water quality issue and replaced it with pure water, but it still rusted. After investigation, the problem lies in the surface condition after high-pressure water impact.

高壓水沖擊會(huì)改變金屬表面的微觀狀態(tài)。
High pressure water impact can alter the microscopic state of metal surfaces.
高壓水射流沖擊零件表面時(shí),不僅沖掉毛刺,還會(huì)對(duì)加工面產(chǎn)生一定的冷作硬化效果。金屬表面在高速水流的反復(fù)沖擊下,晶格發(fā)生畸變,表面能升高,處于一種“活化”狀態(tài)。這種活化表面與空氣中的氧氣接觸后,氧化速度比正常表面快得多。尤其是鋁合金和碳鋼零件,去毛刺后如果不做處理,幾個(gè)小時(shí)內(nèi)就可能出現(xiàn)氧化變色。
When high-pressure water jet impacts the surface of parts, it not only removes burrs, but also has a certain cold work hardening effect on the machined surface. Under the repeated impact of high-speed water flow, the lattice of the metal surface undergoes distortion, the surface energy increases, and it is in an "activated" state. After coming into contact with oxygen in the air, this activated surface oxidizes much faster than a normal surface. Especially for aluminum alloy and carbon steel parts, if not treated after deburring, oxidation discoloration may occur within a few hours.
毛刺沖掉之后,露出的新鮮金屬?zèng)]有保護(hù)。
After the burrs are removed, the fresh metal exposed is not protected.
毛刺本身是金屬,沖掉毛刺意味著原本被毛刺覆蓋的基體金屬暴露出來。這部分金屬?zèng)]有經(jīng)過鈍化處理,也沒有油膜保護(hù),直接暴露在空氣中。如果車間濕度高,或者零件表面殘留水分,銹蝕幾乎是必然的。
The burr itself is metal, and removing the burr means that the base metal originally covered by the burr is exposed. This part of the metal has not been passivated or protected by an oil film, and is directly exposed to the air. If the humidity in the workshop is high or there is residual moisture on the surface of the parts, corrosion is almost inevitable.
防銹處理建議緊跟在去毛刺之后。
Rust prevention treatment must be carried out immediately after deburring.
正規(guī)的工藝流程是:高壓水去毛刺→漂洗→脫水→防銹處理。防銹處理有幾種方式:浸泡水基防銹劑、噴涂防銹油、或者做鈍化處理。水基防銹劑環(huán)保但防銹期短,適合工序間周轉(zhuǎn);防銹油防銹期長但后續(xù)裝配前需要清洗;鈍化處理適合不銹鋼和鋁合金,能形成致密的氧化膜。選擇哪種,取決于零件的材質(zhì)和后續(xù)工序要求。
The formal process is: high-pressure water deburring → rinsing → dehydration → rust prevention treatment. There are several ways to prevent rust: soaking in water-based rust inhibitors, spraying rust proof oil, or performing passivation treatment. Water based rust inhibitors are environmentally friendly but have a short rust prevention period, making them suitable for inter process turnover; Rust proof oil has a long rust prevention period but needs to be cleaned before subsequent assembly; Passivation treatment is suitable for stainless steel and aluminum alloys, and can form a dense oxide film. The choice depends on the material of the parts and the requirements of subsequent processes.
烘干不有效,防銹做了也白做。
The drying is not thorough, and even if rust prevention is done, it is useless.
零件從清洗機(jī)出來后,表面和盲孔里會(huì)殘留水分。如果烘干不有效就噴防銹油,水分被封在油膜下面,反而加速銹蝕。盲孔和深孔的烘干尤其要重視——熱風(fēng)要能吹進(jìn)去,或者用真空干燥的方式把水分抽出來。烘干后的零件表面溫度不能太高,否則噴防銹劑時(shí)溶劑快速揮發(fā),防銹膜不均勻。
After the parts come out of the cleaning machine, there will be residual moisture on the surface and in blind holes. If the drying is not thorough and rust proof oil is sprayed, the moisture will be sealed under the oil film, which will accelerate the rusting process. The drying of blind and deep holes should be particularly emphasized - hot air should be able to blow in, or water should be extracted through vacuum drying. The surface temperature of the dried parts should not be too high, otherwise the solvent will evaporate quickly when spraying rust inhibitor, and the rust proof film will be uneven.
工序間的等待時(shí)間要控制。
The waiting time between processes should be controlled.
去毛刺和防銹之間的等待時(shí)間越短越好。有的車間去毛刺和防銹是兩道獨(dú)立工序,中間零件堆在周轉(zhuǎn)箱里等半天,這半天就足夠碳鋼零件生銹了。理想的做法是把去毛刺、漂洗、防銹、烘干集成在一條線上,零件從一頭進(jìn),從另一頭出來就是防銹狀態(tài)。
The shorter the waiting time between deburring and rust prevention, the better. In some workshops, deburring and rust prevention are two independent processes. The intermediate parts are stacked in turnover boxes and wait for half a day, which is enough time for the carbon steel parts to rust. The ideal approach is to integrate deburring, rinsing, rust prevention, and drying into one line, where parts enter from one end and exit from the other end to achieve rust prevention.
CNC高壓清洗機(jī)解決的是毛刺問題,但去毛刺之后的表面防護(hù)是另一個(gè)環(huán)節(jié)。去毛刺做得再好,防銹跟不上,零件還是要返工。選設(shè)備的時(shí)候,把清洗、漂洗、防銹、烘干作為一個(gè)整體流程來考慮,比只盯著高壓泵的參數(shù)更實(shí)際。
The CNC high-pressure cleaning machine solves the problem of burrs, but surface protection after deburring is another step. No matter how well the deburring is done, the rust prevention cannot keep up, and the parts still need to be reworked. When selecting equipment, considering cleaning, rinsing, rust prevention, and drying as a whole process is more practical than just focusing on the parameters of the high-pressure pump.